This table gives various engineering material properties listed alphabetically. The units are SI.
Go Directly To Property:
Density Heat of vaporization
Elastic modulus Heat transfer coefficient
Electrical resistivity Kinematic viscosity
Heat capacity Poisson's ratio
Heat of combustion Thermal Conductivity
Heat of fusion Thermal expansion coefficient
  Viscosity

[ I realize that there may be errors on this page, if you find one, please contact me]
 
Density Acrylic  1400  kg/m^3 
Density  Air (2800 m)  0.9800  kg/m^3 
Density  Air (STP)  1.2930  kg/m^3 
Density  Aluminum 2024-T3  2770  kg/m^3 
Density  Aluminum 3003  2700  kg/m^3 
Density  Aluminum 6061-T6  2700  kg/m^3 
Density  Aluminum 7079-T6  2740  kg/m^3 
Density  Ammonia - liquid  682.10  kg/m^3 
Density  Argon - liquid  1390  kg/m^3 
Density  Beryllium QMV  1850  kg/m^3 
Density  Borosilicate Ohara E6  2180  kg/m^3 
Density  Borosilicate Tempax  2230  kg/m^3 
Density  Concrete  2242  kg/m^3 
Density  Copper - pure  8900  kg/m^3 
Density  Dow Corning 200 (350cSt)  968.00  kg/m^3 
Density  Fused silica  2200 kg/m^3 
Density  Glass wool  64.00  kg/m^3 
Density  Gold - pure  1.932E+04  kg/m^3 
Density  Helium - liquid  125.00  kg/m^3 
Density  Hydrogen - liquid  70.00  kg/m^3 
Density  Iron  7830  kg/m^3 
Density  Lead - pure  1.134E+04  kg/m^3 
Density  Magnesium AZ31B-H24  1770  kg/m^3 
Density  Magnesium HK31A-H24  1790  kg/m^3 
Density  Methane - liquid  424.00  kg/m^3 
Density  Molybdenum - wrought  1.030E+04  kg/m^3 
Density  Neon - liquid  1200  kg/m^3 
Density  Nickel - pure  8900  kg/m^3 
Density  Nitrogen - liquid  804.00  kg/m^3 
Density  Nylon  1700  kg/m^3 
Density  Platinum  2.145E+04  kg/m^3 
Density  Polycarbonate  1300  kg/m^3 
Density  Polyethylene  2300  kg/m^3 
Density  PTFE  1200  kg/m^3 
Density  SiC Alpha  2975  kg/m^3 
Density  SiC sintered KT  2975  kg/m^3 
Density  Silver - pure  1.050E+04  kg/m^3 
Density  Steel AISI 304  8030  kg/m^3 
Density  Steel AISI C1020  7850  kg/m^3 
Density  Tantalum  1.660E+04  kg/m^3 
Density  Titanium B 120VCA  4850  kg/m^3 
Density  Tungsten  1.930E+04  kg/m^3 
Density  Water (4 C)  999.97  kg/m^3 
Density  White pine  513.00  kg/m^3 
Elastic modulus  Aluminum 2024-T3 7.310E+10  Pa 
Elastic modulus  Aluminum 6061-T6  7.310E+10  Pa 
Elastic modulus  Aluminum 7079-T6  7.172E+10  Pa 
Elastic modulus  Beryllium QMV  2.897E+11  Pa 
Elastic modulus  Borosilicate Ohara E6  5.743E+10  Pa 
Elastic modulus  Borosilicate Tempax  6.200E+10  Pa 
Elastic modulus  Copper - pure  1.172E+11  Pa 
Elastic modulus  Gold - pure  7.448E+10  Pa 
Elastic modulus  Lead - pure  1.379E+10  Pa 
Elastic modulus  Magnesium AZ31B-H24  4.483E+10  Pa 
Elastic modulus  Magnesium HK31A-H24  4.414E+10  Pa 
Elastic modulus  Molybdenum - wrought  2.759E+11  Pa 
Elastic modulus  Nickel - pure  2.207E+11  Pa 
Elastic modulus  Platinum  1.469E+11  Pa 
Elastic modulus SiC Alpha  4.760E+11  Pa 
Elastic modulus  SiC sintered KT  3.320E+11  Pa 
Elastic modulus  Silver - pure  7.241E+10  Pa 
Elastic modulus  Steel AISI 304  1.931E+11  Pa 
Elastic modulus  Steel AISI C1020  2.034E+11  Pa 
Elastic modulus  Tantalum  1.862E+11  Pa 
Elastic modulus  Titanium B 120VCA  1.021E+11  Pa 
Elastic modulus  Tungsten  3.448E+11  Pa 
Electrical resistivity  Aluminum 2017  4.000E-08  ohm*m 
Electrical resistivity  Aluminum 3003  4.000E-08  ohm*m 
Electrical resistivity  Aluminum 99.996%  2.655E-08  ohm*m 
Electrical resistivity  Copper  1.673E-08  ohm*m 
Electrical resistivity  Nickel ASTM B160  1.000E-07  ohm*m 
Electrical resistivity  Steel AISI 304  7.200E-07  ohm*m 
Electrical resistivity  Steel AISI C1020  1.000E-07  ohm*m 
Heat capacity  Air  1006  J/kg*°C 
Heat capacity  Aluminum 2024-T3  963.00  J/kg*°C 
Heat capacity  Aluminum 6061-T6  963.00  J/kg*°C 
Heat capacity  Aluminum 7079-T6  963.00  J/kg*°C 
Heat capacity  Beryllium QMV  1884  J/kg*°C 
Heat capacity  Borosilicate glass  710.00  J/kg*°C 
Heat capacity  Concrete  1000  J/kg*°C 
Heat capacity  Copper - pure  385.00  J/kg*°C 
Heat capacity  Dow Corning 200 (350 cST)  1465  J/kg*°C 
Heat capacity  Ethanol (25°C)  2453  J/kg*°C 
Heat capacity  Gold - pure  130.00  J/kg*°C 
Heat capacity  Ice  2093  J/kg*°C 
Heat capacity  Iron  440.00  J/kg*°C 
Heat capacity  Lead - pure  130.00  J/kg*°C 
Heat capacity  Magnesium AZ31B-H24  1047  J/kg*°C 
Heat capacity  Magnesium HK31A-H24  544.00  J/kg*°C 
Heat capacity  Methanol (25°C)  2547  J/kg*°C 
Heat capacity  Molybdenum - wrought  293.00  J/kg*°C 
Heat capacity  Nickel - pure  461.00  J/kg*°C 
Heat capacity  Platinum  130.00  J/kg*°C 
Heat capacity  SiC Alpha  1300  J/kg*°C 
Heat capacity  SiC sintered KT  1340  J/kg*°C 
Heat capacity  Silica (0°C)  937.00  J/kg*°C 
Heat capacity  Silver - pure  235.00  J/kg*°C 
Heat capacity  Steel AISI 304  503.00  J/kg*°C 
Heat capacity  Steel AISI C1020  419.00  J/kg*°C 
Heat capacity  Tantalum  126.00  J/kg*°C 
Heat capacity  Titanium B 120VCA  544.00  J/kg*°C 
Heat capacity  Tungsten  138.00  J/kg*°C 
Heat capacity  Water  4216  J/kg*°C 
Heat of combustion  Methane  55.70  MJ/kg 
Heat of combustion  Octane  47.70  MJ/kg 
Heat of fusion  Nitrogen  25.50  kJ/kg 
Heat of fusion  Water  334.00  kJ/kg 
Heat of vaporization  Ammonia  1368  kJ/kg 
Heat of vaporization  Argon  162.76  kJ/kg 
Heat of vaporization  Helium  23.93  kJ/kg 
Heat of vaporization  Hydrogen  451.90  kJ/kg 
Heat of vaporization  Methane  577.40  kJ/kg 
Heat of vaporization  Neon  87.03  kJ/kg 
Heat of vaporization  Nitrogen  199.20  kJ/kg 
Heat of vaporization  Water (100°C)  2258  kJ/kg 
Heat transfer coef.  Air v = 0 m/s  5.6000  W/°C*m^2 
Heat transfer coef.  Air v = 3.4 m/s  18.90  W/°C*m^2 
Heat transfer coef.  Air v = 6.7 m/s  38.00  W/°C*m^2 
Kinematic viscosity  Air (101 kPa)  1.800E-05  m^2/s 
Kinematic viscosity  Dow Corning 200 (350cSt)  1.121E-07  m^2/s 
Kinematic viscosity  Water (0°C)  1.753E-06  m^2/s 
Poisson's ratio  Aluminum 2024-T3  0.3300   
Poisson's ratio  Aluminum 6061-T6  0.3300   
Poisson's ratio  Aluminum 7079-&6  0.3300   
Poisson's ratio  Beryllium QMV  0.0300   
Poisson's ratio  Borosilicate Ohara E6  0.1950   
Poisson's ratio  Borosilicate Tempax  0.2200   
Poisson's ratio  Copper - pure     
Poisson's ratio  Gold - pure  0.4200   
Poisson's ratio  Lead - pure  0.4200   
Poisson's ratio  Magnesium AZ31B-H24  0.3500   
Poisson's ratio  Magnesium HK31A-H24  0.3500   
Poisson's ratio  Molybdenum - wrought  0.3200   
Poisson's ratio  Nickel - pure     
Poisson's ratio  Platinum  0.3900   
Poisson's ratio  Silver - pure  0.3700   
Poisson's ratio  Steel AISI 304  0.2900   
Poisson's ratio  Steel AISI C1020  0.2900   
Poisson's ratio  Tantalum  0.3500   
Poisson's ratio  Titanium B 120VCA  0.3000   
Poisson's ratio  Tungsten  0.2800   
Thermal Conductivity  Acetyl  0.2300  W/m*°C 
Thermal Conductivity  Acrylic  0.1400  W/m*°C 
Thermal Conductivity  Aluminum 2024-T3  190.40  W/m*°C 
Thermal Conductivity  Aluminum 3003  233.64  W/m*°C 
Thermal Conductivity  Aluminum 6061-T6  155.80  W/m*°C 
Thermal Conductivity  Aluminum 7079-T6  121.10  W/m*°C 
Thermal Conductivity  Beryllium QMV  147.10  W/m*°C 
Thermal Conductivity  Borosilicate glass  1.1300  W/m*°C 
Thermal Conductivity  Borosilicate glass (Tempax)  1.1300  W/m*°C 
Thermal Conductivity  Concrete (sand & gravel)  1.8000  W/m*°C 
Thermal Conductivity  Copper - pure  392.90  W/m*°C 
Thermal Conductivity  Diamond 550.00  W/m*°C 
Thermal Conductivity  Douglas fir  0.1100  W/m*°C 
Thermal Conductivity  Dow Corning 200 (350cSt)  0.1590  W/m*°C 
Thermal Conductivity  Dow Corning 739  0.1900  W/m*°C 
Thermal Conductivity  Dow Corning 93-500  0.1500  W/m*°C 
Thermal Conductivity  Dow Corning Q3-6605  0.8400  W/m*°C 
Thermal Conductivity  Epoxy (Epotek 353ND)  0.0490  W/m*°C 
Thermal Conductivity  Epoxy (Masterbond 11A0)  1.4400  W/m*°C 
Thermal Conductivity  Glass wool  0.0400  W/m*°C 
Thermal Conductivity  Gold - pure  297.70  W/m*°C 
Thermal Conductivity  Helium  2.7700  W/m*°C 
Thermal Conductivity  Ice  2.2000  W/m*°C 
Thermal Conductivity  Iron  83.50  W/m*°C 
Thermal Conductivity  Lead - pure  37.04  W/m*°C 
Thermal Conductivity  Limestone  0.5000  W/m*°C 
Thermal Conductivity  Magnesium HK31A-H24  114.20  W/m*°C 
Thermal Conductivity  Magnesium AZ31B-H24  95.19  W/m*°C 
Thermal Conductivity  Methane  0.3030  W/m*°C 
Thermal Conductivity  Molybdenum - wrought  143.60  W/m*°C 
Thermal Conductivity  Nickel - pure  91.73  W/m*°C 
Thermal Conductivity  Nitrogen  0.1460  W/m*°C 
Thermal Conductivity  Nylon  0.2400  W/m*°C 
Thermal Conductivity  Platinum  69.23  W/m*°C 
Thermal Conductivity  Polycarbonate  0.2000  W/m*°C 
Thermal Conductivity  Polypropylene  0.4000  W/m*°C 
Thermal Conductivity  Polystyrene foam  0.3600  W/m*°C 
Thermal Conductivity  Polyurethane foam  0.0260  W/m*°C 
Thermal Conductivity  PTFE  0.2400  W/m*°C 
Thermal Conductivity  Quartz  1.3200  W/m*°C 
Thermal Conductivity  SiC Alpha  77.50  W/m*°C 
Thermal Conductivity  SiC sintered KT  80.00  W/m*°C 
Thermal Conductivity  Silastic E  0.1800  W/m*°C 
Thermal Conductivity  Silastic L  0.2800  W/m*°C 
Thermal Conductivity  Silicone foam (Poron)  0.0600  W/m*°C 
Thermal Conductivity  Silver - pure  417.10  W/m*°C 
Thermal Conductivity  Snow (light)  0.6000  W/m*°C 
Thermal Conductivity  Snow (packed)  2.2000  W/m*°C 
Thermal Conductivity  Soil (coarse)  0.5200  W/m*°C 
Thermal Conductivity  Soil (dry w/stones)  0.5200  W/m*°C 
Thermal Conductivity  Soil (dry)  0.2300  W/m*°C 
Thermal Conductivity  Soil (w/42% water)  1.1000  W/m*°C 
Thermal Conductivity  Steel AISI 304  16.27  W/m*°C 
Thermal Conductivity  Steel AISI C1020  46.73  W/m*°C 
Thermal Conductivity  Tantalum  53.65  W/m*°C 
Thermal Conductivity  Titanium B 120VCA  7.4420  W/m*°C 
Thermal Conductivity  Tungsten  164.40  W/m*°C 
Thermal Conductivity  Water  0.6030  W/m*°C 
Thermal Conductivity  White pine  0.1100  W/m*°C 
Thermal expansion coefficient  Aluminum 2024-T3  22.68  µm/m*°C 
Thermal expansion coefficient  Aluminum 6061-T6  24.30  µm/m*°C 
Thermal expansion coefficient  Aluminum 7079-T6  24.66  µm/m*°C 
Thermal expansion coefficient  Beryllium QMV  14.94  µm/m*°C 
Thermal expansion coefficient  Borosilicate E6 -30 to +70C  2.8000  µm/m*°C 
Thermal expansion coefficient  Copper - pure  16.56  µm/m*°C 
Thermal expansion coefficient  Gold - pure  14.4  µm/m*°C 
Thermal expansion coefficient  Lead - pure  52.74  µm/m*°C 
Thermal expansion coefficient  Magnesium AZ31V-H24  26.10  µm/m*°C 
Thermal expansion coefficient  Magnesium HK31A-H24  25.20  µm/m*°C 
Thermal expansion coefficient  Molybvdenum - wrought  5.4000  µm/m*°C 
Thermal expansion coefficient  Nickel - pure  12.96  µm/m*°C 
Thermal expansion coefficient  Platinum  9.0000  µm/m*°C 
Thermal expansion coefficient  SiC Alpha  4.0000  µm/m*°C 
Thermal expansion coefficient  SiC sintered KT  5.0000  µm/m*°C 
Thermal expansion coefficient  Silver - pure  19.80  µm/m*°C 
Thermal expansion coefficient  Steel AISI 304  17.82  µm/m*°C 
Thermal expansion coefficient  Steel AISI C1020  11.34  µm/m*°C 
Thermal expansion coefficient  Tantalum  6.4800  µm/m*°C 
Thermal expansion coefficient Titanium B 120VCA  9.3600  µm/m*°C 
Thermal expansion coefficient  Tungsten  4.5000  µm/m*°C 
Viscosity  Air (0°C,101 kPa)  1.708E-05  N*s/m^2 
Viscosity  Carbon dioxide (0°C,101 kPa)  1.390E-05  N*s/m^2 
Viscosity  Helium (0°C,101 kPa)  1.860E-05  N*s/m^2 
Viscosity  Hydrogen (0°C,101 kPa)  8.345E-06  N*s/m^2 
Viscosity  Methane (0°C,101 kPa)  1.026E-05  N*s/m^2 
Viscosity  Nitrogen (0°C,101 kPa)  1.660E-05  N*s/m^2 
Viscosity  Oxygen (0°C,101 kPa)  1.919E-05  N*s/m^2 
Viscosity  Benzene (0°C)  9.121E-04  N*s/m^2 
Viscosity  Carbon tetrachloride (0°C)  1.346E-03  N*s/m^2 
Viscosity  Glycerin (0°C)  12.07  N*s/m^2 
Viscosity  Kerosene (0°C)  2.959E-03  N*s/m^2 
Viscosity  Mercury (0°C)  1.685E-03  N*s/m^2 
Viscosity  Oil - light machine (0°C)  0.3534  N*s/m^2 
Viscosity  Water (0°C)  1.753E-03  N*s/m^2 


Back to Fred's Engineering Page...

This page created November 21, 1997
Last updated July 28, 2001